All formulations
Formulation Card

FC-13.14-P

Paint Sealant — Spray-On Polymer

Ingredients

Ingredient% w/wFunction
Deionized waterqs to 100.0Diluent
Acrylic/silicone hybrid emulsion (40%)18.0Primary binder, film formation
Silica nanoparticle dispersion (30% SiO₂)5.0Hardness, chemical resistance
UV absorber (hydroxybenzotriazole)1.0UV-A/UV-B absorption
Nonionic surfactant0.5Wetting, leveling
Glycol ether (DPnB)2.0Coalescing aid, film formation
Preservative0.2Microbial protection
Total100.0

Formulation Notes

Acrylic/silicone hybrid sealant for 3–6 month durability with UV protection.

Method: Add hybrid emulsion to water with gentle stirring. Add silica dispersion and UV absorber (pre-dissolved). Add surfactant and glycol ether. Add preservative. Properties: pH 7.0–8.5, translucent liquid, viscosity 200–500 cP. The acrylic/silicone hybrid binder combines the adhesion and gloss of acrylics with the hydrophobicity and flexibility of polydimethylsiloxane . Silica nanoparticles (20–50 nm) create micro-roughness on the cured film that enhances water beading (contact angle > 110°). UV absorber at 1.0% provides equivalent protection to SPF 30+ sunscreens, preventing clear-coat oxidation and fading . Application: spray and wipe; allow 24 hours for full cure before exposure to water.